- Density
- 1,8 g/cm3
- Compressibility (ASTM F 36 J)
- 9 %
- Recovery (ASTM F 36 J)
- 55 %
- Hot stress relaxation — DIN 52913 (50 MPa, 16 h/175°C)
- 39 MPa
- Hot stress relaxation — DIN 52913 (50 MPa, 16 h/300°C)
- 35 MPa
- Relaxation — BS 7531 (40 MPa, 16h/300°C)
- 31 MPa
- Cold/hot compression (KLINGER, 50 MPa)
- 8% at 23°C / 11% at 300°C
- Sealing (DIN 28090-2)
- 0,05 mg/(s·m)
- Specific leakage rate (VDI 2440)
- 2,13 x 10-5 mbar·l/(s·m)
- Swelling after immersion (ASTM F 146)
- IRM 903 oil (5 h/150°C): 3% — Fuel B (5 h/23°C): 5%
- Thermal conductivity
- 0,38 W/mK
- Classification (BS 7531:2006)
- Grade AX
- ASME gasket factors at 2 mm thickness
- y = 20 MPa / m = 1,6
- Optimum operating conditions
- 0 – 40 bar / -150°C to +250°C